Adhesion Testing of Hauthane Polyurethane Dispersions (un-pigmented) on Various Substrates

This table shows the results of adhesion testing of 12 Hauthane Polyurethane Dispersions on 8 substrates.  Coatings were applied to IPA wiped substrate via #100 WWR, followed by 30 minutes drying time at 180°F (82°C).  Adhesion was tested on cooled panels via the cross-hatch test (ASTM D3359, Method B).  Results are reported on a scale of 0B to 5B in accordance with the ASTM method.  See below for an explanation of the reporting scale.

 

ABS
(Magnum 344
HP)
Polyphenylene-
oxide (PPO)
(GE Noryl PX
0844-780)
Polycarbonate
(GE Lexan
EM 1210)
Polypropylene
(Mytex
AX03B)
Polypropylene
(Montell
Profax)
PPO/Nylon
Alloy (GE
Noryl GTX
910 71653)
Polystyrene
(DOW
Styron 478)
Acrylic (ELF
ATOCHEM
V825-100)
HD-2007 5B 0B 5B 0B 0B 5B 0B 0B
HD-2101 5B 0B 5B 0B 0B 5B 0B 0B
HD-2107 5B 0B 5B 0B 0B 5B 0B 0B
HD-2015 1B 0B 0B 0B 0B 5B 0B 0B
HD-2113 0B 0B 0B 0B 0B 0B 0B 0B
HD-2139 0B 0B 0B 0B 0B 4B 0B 0B
HD-2209 5B 0B 5B 0B 0B 0B 0B 0B
HD-3011 5B 0B 5B 0B 0B 5B 0B 0B
HD-2314 0B 0B 0B 0B 0B 5B 0B 0B
HD-4664 0B 0B 5B 0B 0B 0B 0B 5B
HD-4669 0B 0B 0B 0B 0B 5B 0B 1B
HD-5002 5B 5B 5B 0B 0B 5B 5B 5B

 

Classification Approximate percentage of cross cut area from which flaking has occurred
5B 0
4B <10%
3B 10-20%
2B 20-40%
1B 40-65%
0B >65%

 

REACH Pre-Registration Notice
Hauthaway is fully compliant with the pre-registration requirements of REACH.
All substances in our polyurethane products and all monomers used to make our polymers have been pre-registered.
Have Questions? Call us at 781-592-6444 or contact our distributors Let's discuss the possibilities.
Email: info@hauthaway.com